Things You'll Need
Instructions
Mix the aluminum oxide and chromium oxide powders together. Place the powdered mixture in the hopper of the Verneuil furnace, which is the container at or near the top of the blowpipe.
Connect the oxygen tank to the uppermost valve on the furnace blowpipe and the hydrogen valve on the lower valve of the furnace blowpipe. Turn the hydrogen tank on and press the ignite button on the furnace, near the hydrogen valve nozzle. Then, turn the oxygen tank on, releasing oxygen to fuel the hydrogen fire within the blowpipe.
Start the hammer at the top of the furnace blowpipe. Set its speed to 80 taps per minute. It will release the powdered mixture down the blowpipe shaft into the hydrogen flame. There, the powder will molten, dripping onto the ceramic pedestal below and creating the synthetic ruby. After about ten minutes, or when a suitable base has formed on top of the ceramic pedestal, reduce the speed of the hammer to 20 taps per minute.
Cut off the gas supply when all of the powder has been released, after about two or three hours. Allow the ceramic pedestal and synthetic ruby, or boule, to cool overnight.
Remove the boule from the furnace. Give the ruby end a slight tap with a hammer, which will cause it to split in half and disconnect from its ceramic base.