Things You'll Need
Instructions
Use a Bunsen burner to heat 3 level teaspoons magnesium powder mixed with 3 level teaspoons clean, dry sharp sand (not sand from a beach because of salt contamination) in a test tube. Wear heat-proof gloves if necessary. The magnesium takes oxygen atoms from the sand, leaving elemental silicon along with magnesium, magnesium oxide and magnesium silicide.
Remove from heat priot to purifying the mixture with an acid solution.
Pour 5 cups of cold water into a large laboratory flask. Add 1 cup of muriatic acid. Do not reverse these steps -- the acid must be added to the water.
Let the test tube cool for five minutes. Add the contents to the flask, using a funnel if the flask mouth is not wide enough. The reaction will be vigorous; therefore, place the flask on a worktop rather than holding it.
Allow the bubbling, foaming and fumes to settle, which should take less than one minute. The remains in the bottom of the flask are silicon crystals.